行业资讯
水稳料怕“等”,摊铺慢一步就废
济南工地做道路基层,水稳料进场看着都一个样——灰白、湿润、翻斗车倒下来堆成小山。可同样一车料,有的压实度轻松过 98%,有的钻芯取出来一捏就散。差别往往不在级配,在“时间”和“含水”这两条线上没卡住。
At the construction site in Jinan, the road base is being built, and the water stable materials entering the site look the same - gray and white, moist, and piled up into small hills by dump trucks. However, for the same batch of materials, some can easily achieve a compaction degree of over 98%, while others can easily scatter the drill core when pinched. The difference often lies not in the grading, but in the two lines of "time" and "moisture content".

水稳是水泥稳定碎石的简称,靠水泥水化把碎石胶结成半刚性板体。它有两个硬时钟:初凝时间和允许延迟时间。普通硅酸盐水泥初凝一般 3 小时上下,水稳从拌合到突出完成,规范卡在 2 小时内、非常好压完不超初凝。夏天济南中午地表 40℃,摊铺机前面等料、压路机后面等降温,一车料从拌合站出来到压完超过 3 小时,水泥已经开始初凝,再压就是“压碎已结的胶”,强度直接掉一档。
Water stable is the abbreviation for cement stabilized crushed stone, which is bonded into a semi-rigid plate by cement hydration. It has two hard clocks: initial setting time and allowable delay time. The initial setting time of ordinary Portland cement is generally around 3 hours, and the water stabilization process is completed from mixing to rolling. The standard is to hold it within 2 hours, and it is best to complete the rolling process within the initial setting time. At noon in summer in Jinan, the ground temperature drops to 40 ℃. The temperature drops in front of the paver and behind the roller. After a truck of materials leaves the mixing station and is pressed for more than 3 hours, the cement has already started to set. Pressing it again is called "crushing the already solidified glue", and the strength drops by one level.
含水率也是命门。非常佳含水率靠击实试验定,现场摊铺时要比非常佳值高 0.5%–1%——因为摊铺、倒运、刮平全程在蒸发。济南春秋风大,一车料 20 分钟不盖篷布,表面就干一层白,下面湿上面干,压路机一过起皮。反过来雨天进场含水超标,细料被冲走、级配跑偏,压实度再高也白搭。
Moisture content is also a destiny. The optimal moisture content is determined by compaction tests, and during on-site paving, it should be 0.5% -1% higher than the optimal value - because the entire process of paving, transportation, and leveling evaporates. Jinan's spring and autumn winds are strong. If a truck of materials is not covered with tarpaulin for 20 minutes, the surface will dry to a layer of white, the bottom will be wet and the top will be dry, and the roller will peel off once it passes. On the other hand, if the water content exceeds the standard during rainy days, the fine materials will be washed away, the grading will deviate, and no matter how high the compaction degree is, it will be useless.
进场验收别只看“灰不灰”。抓一把捏:能成团、松手轻碰散开,接近非常佳;一捏出水是过湿;捏不成团、手上沾白灰是水泥多或已初凝。再翻车斗底看有没有离析——粗料滚两边、细料堆中间,摊铺机螺旋布料前不处理,基层就出“砂窝”和“石窝”,面层铺上去半年就反射裂缝。
Don't just look at whether it's gray or not when entering the site for acceptance. Grasp and pinch: can form a ball, release and lightly tap to disperse, approaching the best; When squeezed, the water is too wet; The inability to form a ball or the presence of white ash on the hands indicates that there is too much cement or it has already set. Check for segregation at the bottom of the dumping bucket again - if the coarse material rolls on both sides and the fine material pile is not treated before the spreading machine spirals the fabric, "sand pits" and "stone pits" will appear on the base layer, and if the surface layer is laid for six months, it will reflect cracks.
摊铺段长也要算。水稳摊铺机速度别贪,一段 200–300 米摊完立刻上压路机跟压,别摊 500 米再回头压。跟压顺序:先静压 1 遍排气 → 高频低幅振压 3–4 遍到压实度 → 非常后静压收面。压完立刻覆土工布或薄膜洒水养生 7 天,济南冬天夜间零下,养生不到位,第二天表面就起砂、7 天钻芯取不出完整芯样。
The length of the paving section should also be taken into account. Don't be greedy for the speed of the water stable paver. After a section of 200-300 meters is spread, immediately put it on the road roller to follow, don't spread it for 500 meters and then turn back to press. Follow the pressure sequence: First, static pressure is applied once for exhaust, then high-frequency and low amplitude vibration pressure is applied 3-4 times until the compaction degree is reached, and finally static pressure is applied to the surface. Immediately cover with geotextile or film and sprinkle water for 7 days of curing after pressing. In Jinan, the temperature drops below zero at night during winter, and if the curing is not in place, the surface will start to sand the next day, and a complete core sample cannot be obtained after 7 days of drilling.
还有个隐账:井盖周边和纵横接缝。水稳跟井圈交接处非常容易漏压,机械压不到就人工夯,夯完拿 3 米直尺靠一下,差超 5mm 面层铺完必跳车。隔天接茬要切垂直缝、刷水泥浆搭接,别斜着糊上去。
There is also a hidden account: the perimeter of the manhole cover and the longitudinal and transverse seams. The junction between water stability and well circle is most prone to pressure leakage. If mechanical pressure cannot reach it, manual compaction is necessary. After compaction, use a 3-meter ruler to lean against it. If the surface layer is more than 5mm away, the vehicle must be skipped. The next day, vertical joints should be cut and cement paste should be applied to overlap. Do not apply it diagonally.
水稳料不是“倒下去压平就行”的料。拌完 2 小时内压完、含水比非常佳高半点、摊完跟压、养生 7 天——这四条咬住,济南这边的基层才真能扛住面层和车轮,不然铺得再平,也是给半年后的裂缝攒素材。
Water stable material is not a material that can be poured down and flattened. After mixing, press it within 2 hours, increase the water content by half to the optimal level, spread and press it, and maintain it for 7 days - these four measures are crucial for the base layer in Jinan to withstand the surface layer and wheels. Otherwise, even if it is laid flat, it will still accumulate material for cracks that may occur six months later.
本文由济南水稳料友情奉献。更多有关的知识请点击:http://www.ycgjglcl.com 我们将会对你提出的疑问进行详细的解答,欢迎你登录网站留言.
This article is contributed by Jinan Water Stable Material Friendship. For more information, please click: http://www.ycgjglcl.com We will provide detailed answers to your questions. You are welcome to log in to our website and leave a message




























公司地址:济南市商河县贾庄镇民营经济创业园
公司名称:永诚广建公路材料(山东)有限公司
备案号: